Dry-Looking Plastic Sheets and High Concrete RH: A Case Study

An anonymized learning summary from a CMM inspection by Brian Prusik, NWFA Certified Wood Flooring Inspector and ICRI Certified Concrete Slab Moisture Testing Technician.

Can a concrete floor look dry under plastic and still have elevated internal moisture? In this residential replacement-floor project, both conditions were recorded. The case shows why a visual observation should not replace the testing required for the selected flooring system.

The project question

The original flooring had been removed and portions of the concrete had been skim coated. A new floating rigid-core floor was planned. Small plastic-covered areas appeared generally dry, with no obvious visible condensation at the time of observation.

What the moisture readings showed

  • Test location 1: 89.4% RH.
  • Test location 2: 88.0% RH.
  • Test location 3: 86.2% RH.
  • Test location 4: 87.3% RH.

The recorded range was 86.2% to 89.4% RH, averaging approximately 87.7%. The report treated this as elevated internal slab moisture across the tested areas. Those readings described the locations and conditions tested; they did not establish the condition of every part of the slab.

Why the dry-looking plastic did not settle the question

The absence of visible condensation was a surface observation. The in-situ probes provided numerical information from inside the concrete. The source report did not treat the informal plastic observations as a substitute for quantitative testing or as proof that the floor was ready to cover.

For the purpose and limits of in-situ testing, see ASTM F2170 concrete relative humidity testing. The method selected for acceptance must match the flooring and installation-product requirements.

A critical distinction: RH versus a manufacturer’s acceptance limit

The flooring instructions reviewed for this project specified a calcium-chloride moisture test and did not provide an RH acceptance limit in the reviewed pages. CMM therefore used the RH readings to characterize the slab condition and inform the proposed moisture-control approach. The report did not invent an RH pass/fail limit for that product.

A numerical result from one test method should not be relabeled as a result from a different method. Where a specification calls for another test, resolve that requirement with the appropriate project parties before accepting the substrate.

Moisture was only part of the installation plan

The report also identified ridges, patch transitions and perimeter irregularities requiring correction. The replacement plan addressed substrate preparation, flatness verification, moisture control and the movement space required for the floating floor. It distinguished manufacturer requirements from additional CMM recommendations.

This is where site-specific flooring specifications help: they connect the observations, selected products and sequence of work instead of treating a moisture reading as the entire installation decision.

The practical lesson

  • Keep the actual readings and test methods in the project record.
  • Obtain current instructions for the exact flooring and installation products.
  • Resolve moisture acceptance, flatness and perimeter movement before installation.
  • Do not assume that a waterproof floor covering removes the need to evaluate the substrate.

This is a summary of the documented evaluation and proposed installation approach. It does not claim that the replacement installation was completed or that a later performance outcome was verified.